The invention discloses a fine-grained magnetite sealed dry waste polishing process, the process comprises the following steps: A, from crushed magnetite ore in screening 5mm magnetite ore, after drying, after breaking up by a screw conveyor screw into the dry separator full sealed dry discarding waste, dumping waste, yield the grade is controlled by the speed of spiral dry separator, dry tailings grade pre qualified tailings grade requirements; B, sealed dry discarding waste tailings by primary screw conveyer to the tailing bin, pre concentrate by screw conveyor sent to the grinding processing system. The invention of the 5mm magnetite dry dumping waste treatment, eliminate the waste rock, the rock into the grinding system, prevent the occurrence of ore with waste thrown phenomenon, reduce the grinding cost, solve the problems affecting iron phyllite, Jasper beneficiation index; pre dumping waste high efficiency, good effect, can control the polishing iron ore containing waste waste, to avoid the waste of resources.
【技术实现步骤摘要】
一种细粒级磁铁矿全密封干式抛废工艺
本专利技术属于矿物加工
,具体涉及一种细粒级磁铁矿全密封干式抛废工艺。
技术介绍
磁铁矿露天开采时贫化率约为3%左右,井下开采时贫化率约为8%,也就是说,采出矿石中含有3-8%的围岩,+5mm块矿采用磁滑轮干式预选,能够将围岩抛出,而-5mm粉矿采用磁滑轮、跳汰干式预选均达不到抛废率80%以上的指标,一是-5mm粉矿含有7%左右的水分,影响了干选指标;二是围岩与磁铁矿比重差小,跳汰干选效果不理想。不预选就造成围岩进入磨选系统,使得磨选成本上升;强行预选,会造成部分矿石随围岩一同抛出,导致资源被浪费。同时,存在-5mm细粒级粉矿磁滑轮、跳汰干式预选粉尘大的问题。
技术实现思路
本专利技术的目的是为了解决现有技术中存在的技术问题,提供一种抛废效果好、抛废效率高,能杜绝废石、围岩进入磨选系统的细粒级磁铁矿全密封干式抛废工艺。为了达到上述目的,本专利技术采用以下技术方案:一种细粒级磁铁矿全密封干式抛废工艺,该工艺包括以下步骤:A、从破碎后磁铁矿石中筛分出-5mm磁铁矿粉矿,经烘干、打散后由螺旋输送机送入螺旋干式磁选机进行全密封干式预选 ...
【技术保护点】
一种细粒级磁铁矿全密封干式抛废工艺,其特征在于该工艺包括以下步骤:A、从破碎后磁铁矿石中筛分出‑5mm磁铁矿粉矿,经烘干、打散后由螺旋输送机送入螺旋干式磁选机进行全密封干式预选抛废作业,抛废产率、品位由螺旋干式磁选机转速控制,干式预选尾矿品位符合合格尾矿品位要求;B、全密封干式预选抛废后预选尾矿由螺旋输送机送入尾矿仓,预选精矿由螺旋输送机送至磨选系统处理。
【技术特征摘要】
1.一种细粒级磁铁矿全密封干式抛废工艺,其特征在于该工艺包括以下步骤:A、从破碎后磁铁矿石中筛分出-5mm磁铁矿粉矿,经烘干、打散后由螺旋输送机送入螺旋干式磁选机进行全密封干式预选...
【专利技术属性】
技术研发人员:展仁礼,王欣,边立国,郭忆,杏仲全,王建平,
申请(专利权)人:甘肃酒钢集团宏兴钢铁股份有限公司,
类型:发明
国别省市:甘肃,62