The invention belongs to the technical field of clothes hanger processing. The manufacturing method of an Eucalyptus clothes rack includes the following steps: (1) removing the crown of the Eucalyptus tree, pressing and peeling, cutting the Eucalyptus into square boards of different lengths according to the required specifications and lengths; (2) freezing the eucalyptus wood in a freezing device; (3) soaking the eucalyptus wood in a crack-proof and moth-proof soaking solution and vacuum drying; (4) putting the dried Eucalyptus into a four-sided planer, shaving and then cutting the eucalyptus wood out. The left shoulder of the hanger and the right shoulder of the hanger; (5) Connect the left shoulder of the hanger with the upper end of the right shoulder of the hanger. After hot pressing, the main body of the hanger is cut and the non-smooth edges are aligned, imitated, polished, polished, drilled and ridged. A smooth hanger body is obtained. The hanger is painted, deodorized and flocked, and then the hook is installed. The invention can solve the problems of easy warping, deformation and cracking of the existing Eucalyptus clothes hanger, and easy to produce mildew spots and worms.
【技术实现步骤摘要】
一种桉木衣架的制作方法
本专利技术属于衣架加工
,具体涉及一种桉木衣架的制作方法。
技术介绍
桉树生长迅速,轮伐周期短,是我国重要的人工林树种。因桉树具有易变形开裂、尺寸稳定性差等缺点,使其应用范围受到限制,目前大部分的桉树人工林木材还是主要用于造纸业的生产,木材加工业对桉树的利用则一直处于落后水平。特别是在桉木衣架的加工制造行业中,由于桉木材质不坚韧,加工使用时容易断,使用寿命不长,长期以来,桉木衣架的市场份额都非常小,尤其是高品质的桉木衣架中更没有其存在。现有的桉木衣架的制造方法是将原木锯成坯板后,直接对坯板进行干燥,然后整形加工,接着上漆和烘干后得到成品。这种技术方案制造得到桉木衣架废品率高,成品容易产生翘曲、变形,出现裂缝及产生霉点,甚者还会有白蚁等蛀虫侵蚀。原木在锯解和干燥中易开裂和变形,出材率低,制品尺寸稳定性差,从而影响桉木衣架的加工和使用。
技术实现思路
本专利技术的目的在于提供一种桉木衣架的制作方法,该方法可以解决现有桉木衣架存在的易翘曲、变形和开裂,以及易产生霉点和虫蛀的问题。为了解决上述问题,本专利技术采用的技术方案是:一种桉木衣架的制作方法,其特征在于,包括如下步骤:(1)采伐种植10~15年的桉树,桉树伐倒后留冠置于阴凉处放置5~7d后,将桉树去冠,压刨去皮,按需要的规格长度切割成不同长度的板方型的桉木;(2)将桉木放入冷冻装置,在温度为-15℃的常压下冷冻15~18h,用空气真空泵降低冷冻装置内的环境压力,并维持在6-12Pa,控制冷凝温度为-30~-20℃,冷冻3~5h后取出晾至25℃;(3)将桉木置于防裂防蛀浸泡液中边搅拌 ...
【技术保护点】
1.一种桉木衣架的制作方法,其特征在于,包括如下步骤:(1)采伐种植10~15年的桉树,桉树伐倒后留冠置于阴凉处放置5~7d后,将桉树去冠,压刨去皮,按需要的规格长度切割成不同长度的板方型的桉木;(2)将桉木放入冷冻装置,在温度为‑15℃的常压下冷冻15~18h,用空气真空泵降低冷冻装置内的环境压力,并维持在6‑12Pa,控制冷凝温度为‑30~‑20℃,冷冻3~5h后取出晾至25℃;(3)将桉木置于防裂防蛀浸泡液中边搅拌边浸泡6~8h,然后将桉木取出送入蒸汽热风烘房内真空干燥,在8~10kPa的环境压力下,先升温至35~38℃并保持45~60min,再升温至40~45℃,待桉木含水率降至13.5~15.5%结束真空干燥;(4)将烘干后的桉木放入四面刨机中刨削平整,然后将桉木切出衣架左肩部和衣架右肩部;(5)衣架左肩部和衣架右肩部相互榫接,且在衣架左肩部和衣架右肩部连接的相对面上均匀涂布一层压敏胶,通过压敏胶粘连衣架左肩部和衣架右肩部,经过热压成型后,按照所需规格尺寸,裁剪成衣架主体,对裁剪后的衣架主体不光滑的边角进行齐头尾、仿形、打磨、抛光、钻眼和打坎,得到平滑的衣架主体,对衣架主体进 ...
【技术特征摘要】
1.一种桉木衣架的制作方法,其特征在于,包括如下步骤:(1)采伐种植10~15年的桉树,桉树伐倒后留冠置于阴凉处放置5~7d后,将桉树去冠,压刨去皮,按需要的规格长度切割成不同长度的板方型的桉木;(2)将桉木放入冷冻装置,在温度为-15℃的常压下冷冻15~18h,用空气真空泵降低冷冻装置内的环境压力,并维持在6-12Pa,控制冷凝温度为-30~-20℃,冷冻3~5h后取出晾至25℃;(3)将桉木置于防裂防蛀浸泡液中边搅拌边浸泡6~8h,然后将桉木取出送入蒸汽热风烘房内真空干燥,在8~10kPa的环境压力下,先升温至35~38℃并保持45~60min,再升温至40~45℃,待桉木含水率降至13.5~15.5%结束真空干燥;(4)将烘干后的桉木放入四面刨机中刨削平整,然后将桉木切出衣架左肩部和衣架右肩部;(5)衣架左肩部和衣架右肩部相互榫接,且在衣架左肩部和衣架右肩部连接的相对面上均匀涂布一层压敏胶,通过压敏胶粘连衣架左肩部和衣架右肩部,经过热压成型后,按照所需规格尺寸,裁剪成衣架主体,对裁剪后的衣架主体不光滑的边角进行齐头尾、仿形、打磨、抛光、钻眼和打坎,得到平滑的衣架主体,对衣架主体进行上漆处理,上漆干燥后,将衣架主体放入低温等离子发生器中除味3~5min,调节低温等离子发生器浓度为2.5~4.5ppm,然后将衣架主体静电喷胶植绒,再将挂钩安装在衣架主体上,即可得到衣架。2.根据权利要求1所述的一种桉木衣架的制作方法,其特征在于:所述防裂防蛀浸泡液由下述方法制备:按重量份计,将10~15份氯化钠、5~10份亚麻油、10~15份氯化钙、5~10份百菌清、10~15份茶籽油和30~45份乙醚混合均匀后,放入反应器中,在温度为35~40℃、搅拌速度为80~120r/min和超声波频率为2500~...